CD Skripsi
Identifikasi Fase Magnetik Dan Komposisi Elemen Pasir Sungai Rokan Sebagai Fungsi Waktu Ball Milling
ABSTRACT
Identification of magnetic particles and the elemental composition of the
natural sands of the Rokan River, Riau Province has been done. The natural sand
samples that have been dried under the sun were separated between magnetic and
non-magnetic particles using Iron Sand Separator (ISS). This result was called
the product of ISS. The product of the ISS was milled using ball milling with iron
balls having diameter of 1.5 cm for 30 hours and 100 hours. The results of this
process were separated using Neodynium Iron Boron (NdFeB) magnets and this
result is called ball milling product. The magnetic susceptibility was calculated
based on the values of magnetic induction (Bo) of a solenoid of 2500 turns, 10 cm
long and 3 cm in dimater and total magnetic induction of the solenoid (BT). The
magnetic induction the solenoid was measured using Pasco Magnetic Probe PS
2160. The results show that the magnetic susceptibility increases from 1140.59 ×
10-5 to 15495.71 × 10-5 for natural sand and ball milling product for 100 hours,
respectively. The X-Ray Fluorescence (XRF) test shows that the composition of
the magnetic element Fe increases from 1.67% to 35.39% for natural sand and
bal milling product of 100 hour, respectively.The X-Ray Diffraction (XRD) test
shows that the magnetic phase of 100 hours ball milling product has a hematite
phase (α-Fe2O3) with some impurities such as silicon (Si) and Titanium (Ti)
Keywords: Natural sand, Ball milling, magnetic induction, magnetic susceptibility
X –Ray Diffraction.
Tidak tersedia versi lain